Tuesday, April 9, 2013

RE: [MW:17316] PWHT for P15E to P3

Sorry  Buttering should be of P3 material i.e. 80SD2 on P91 say thk of 6mm
 
However  PQR to be qualified accordingly i.e
If Carried on Pipe then On P91 pipe at the weld edge butter by P3 material
ii) This buttered pipe to be PWHT at 730 same as on the job
iii) Weld a same PQR coupon i.e One pipe of P91 with buttered and PWHT at 730 and second pipe of P3 material and Joint the same with P3 Filler
This coupon of PQR to be tested w/o PWHT
This will satisfy your all condition
 
Regards
Hegde
 
Hegde
--- On Mon, 8/4/13, Binoy Soman <binoy.spp@DAELIM.CO.KR> wrote:

From: Binoy Soman <binoy.spp@DAELIM.CO.KR>
Subject: RE: [MW:17312] PWHT for P15E to P3
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Date: Monday, 8 April, 2013, 4:42 PM

Thanks Hedge,

 

Buttering shall be with P91 filler? If so, kindly explain the basic technical reason.

 

S.Binoy

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Prakash Hegde
Sent: Monday, April 08, 2013 12:55 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:17311] PWHT for P15E to P3

 

Dear Mr Binoy

i) As per ASME code  P3 Gr 1,2 does not require PWHT if its thk is less than 16mm and For Gr3 It is manadatory for any thk and temp is  min 593 C

ii) For P15E (P91) the PWHt is mandatory at 730C

 

Now if the weld joint  P15E to P3 undergoesPWHT at 730C temp It will be afftecting the  mechanical properties of P3 ( C% 0.5 Mo)

Therefore My openion is Better butter the weld edge of P15E with suitable  P91 filler and

conduct the PWHT of P15E (P91)as  per code at 730C and later on weld that edge with P3 (C % 0.5Mo) consumable and that joint need not be PWHT if it is P3 Gr1 or 2  In this case re is no deteoriation of P3  properties 

However PQR  require to be qualified with above condition

 

Regards

Hegde

 


 C
--- On Mon, 8/4/13, Binoy Soman <binoy.spp@DAELIM.CO.KR> wrote:


From: Binoy Soman <binoy.spp@DAELIM.CO.KR>
Subject: [MW:17309] PWHT for P15E to P3
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Date: Monday, 8 April, 2013, 1:44 PM

Dear experts,

 

Kindly explain about PWHT requirement while welding two materials among which one require PWHT by code and  other does not (Eg; P15E  to P3 materials).

What should be the cycle that must be followed, Is it the same that of P 15E to P 15E?. Considering the lower critical temperature of P3 material , I select 700-730°C temperature range for PWHT of  P15E to P3 (correct me if I am wrong).  

P15E to P15E PWHT cycle that we are following is attached.

 

 

S.Binoy

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...