Please refer UG-84(h)(2) of ASME Sec VIII Div.1'Ed'2010.
If impact testing is required in weld & HAZ when required by UCS-67,
the following shall apply.
For vessels constructed to the rules of part UCS, the test plate
material shall sitisfy all of the following requirements relative to
the material to be used in production.
(a) be of the same P-Number and Group Number;
(b) be in the same heat treated condition; and
(c) meet the minimum notch toughness requirements of UG-84(c)
(4) .......................
Means, one way or other, If you are using LTCS material for production
and requires notch touchness of weld and HAZ then the base material
used for Procedure shall be of same P No..(You can use ASTM A333 Gr.
6(P1G1) to ASTM A350LF2(P1G2) procedure) but you can not use ASTM A106
Gr.B even though it is P1G1 since it "is not the same heat treated
condition" as that of A333 gr.6.
Hope this will clarify!
Cheers!
Raj
On Apr 17, 4:37 pm, Vino Varghese <vinopvargh...@gmail.com> wrote:
> Dear All,
>
> Design Code: ASME Sec VIII, Div 1
> U-Stamp Pressure Vessel
>
> Reference Code : ASME Sec IX, Edition 2007, Add 09
> Material of Construction: SA 516 Gr 70N(30mm thk)
> PQR Material : *1. Pipe* - ASME SA 333 and *2. Flange* : ASTM A350 LF2
>
> *Query:*
> *Is it mandatory that Qualification has to be done only with a ASME
> Material? *
> *If ASTM Material is used for qualification, then WPS will be qualified only
> for that particualr Material and cannot be Qualified as P1 Material. Please
> provide all reference from Code for justification*.
>
> Hope to see that i was able to communicate properly with regard to raised
> query.
>
> Expecting as usual response from all sides.
>
> Thanks & Regards
> Vino-Doha
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment